配方類型: METALS
配方說明: Rhodium Plating
配方組成: Sulphuric acid, C.P./100 ml
For 0.0003 in. + Plat
Replenishment, 5 g/per 4.5 amp.-hr
Replenishment, 5 g/per 5 amp.-hr
Distilled water/to make 1 gal
Rhodium sulphate TP/20 g
Rhodium sulphate TP/40 g
Sulphuric acid, C.P./100 ml
Current density/10-50 ASF
Distilled water/to make 1 gal
Current density/10-40 ASF
配制方法: Tank: Glass, plastic-lined steel ("Koroseal"), rigid PVC such as "Boltaron" and "Lucite".
Anodes: Platinum or Platanodes (0.04-in. platinum-plated titanium sheet). Anode to cathode ratio, 1/2 to 1 minimum, preferably 1 to 1.
Leach all plastic tanks and especially cemented lucite joints, with warm (130F) 10% by volume sulfuric acid for 24 hr. Rinse well. Fill the clean tank half full with distilled or deionized water. Add the required amount of reagent-grade sulfuric acid slowly, with agitation. Mix well.
Add the rhodium sulfate TP with stirring. Mix well.
Add distilled water to bring liquid level to operating volume. Mix well.
Operating Data Temperature Agitation Concentration Current Density