日韩性爱女同性恋,玖玖综合日,不卡啪啪视频,4月婷久久,精品在线观看视频,亚洲一区精选自拍,日韩欧美人妻网站一区,麻豆精品视频一区二区,色尚和久久

化學配方數(shù)據(jù)庫
配方類型: METALS
配方說明: Etchants for Printed Circuits
配方組成: Water/62-60
No.1
Water/902
Catalyst/48
Sodium dichromate/750
Sulfuric acid (93.19%)/1650
Water/870
Catalyst/80
Sodium dichromate/750
Sulfuric acid (93.19%)/1650
Water/2335
Catalyst/20
Chromic acid/385
Sulfuric acid (93.19%)/610
Water/2295
Catalyst/20
Chromic acid/400
Sulfuric acid (93.19%)/400
Water/2215
Catalyst/20
Chromic acid/385
Sulfuric acid (93.19%)/730
Ammonium persulfate/25
Water/2068 <
配制方法: In preparing etchants employing sulfuric acid, it is beneficial to dilute the concentrated acid with at least part of the water first, followed by a standing period to dissipate the appreciable heat of dilution. Or the concentrated acid can be replaced with an equivalent amount of 50% or 60% acid. The sulfuric acid should be added last, after the other materials are in solution.
The formulas shown are typical of this type of product. The theoretical amount of sulfuric acid, required to utilize the chromic acid present, will be seen to range from about 50% ot the calculated amount to about 75% of this figure. Three moles of sulfuric acid are required per mole of chromic acid anhydride. However, if the theoretical amount of sulfuric acid is used, the etchant tends to run wild. Where anything above 75% theoretical sulfuric acid is used, the etchant must be tailor-made to fit a specific etching job.